MEMSnet Home: MEMS-Talk: Ti etchant with selectivity to Al(0.5%Cu)
Ti etchant with selectivity to Al(0.5%Cu)
2003-08-01
Lin, Yaojian
2003-08-04
David Ovrokzky
2003-08-04
Rick Morrison
Ti etchant with selectivity to Al(0.5%Cu)
Rick Morrison
2003-08-04
Hi,
Try 95% H2O2 and 5% NH4OH, this is a very fast etch and resist may or maynot
survive.

Rick


-----Original Message-----
From: [email protected]
[mailto:[email protected]]On Behalf
Of Lin, Yaojian
Sent: Friday, August 01, 2003 12:28 PM
To: 'General MEMS discussion'
Subject: [mems-talk] Ti etchant with selectivity to Al(0.5%Cu)


Dear Friends,

I am working on the etchant for 1000A Ti with selectivity to Al(0.5%Cu). I
tried to use diluted (100:1) HF. But it didn't work.

Could you please give me some help?

With many thanks,

Yaojian Lin



_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
The Branford Group
Process Variations in Microsystems Manufacturing
Harrick Plasma, Inc.