MEMSnet Home: MEMS-Talk: Electropolishing 416 SS
Electropolishing 416 SS
2004-11-15
Charles Becnel
2004-11-16
Amrit Panda
Electropolishing 416 SS
Amrit Panda
2004-11-16
Charles,
To electropolish SST, you are looking at a phosphoric acid based bath.

There are a few possibilities exist

1. Phosphoric acid -50 %
2. Glycerine - 50 %

Current density - 20 ASF, Temp = 200 F

or

Phosphoric acid - 50%
Sulfuric acid - 15%
current density =  50 ASF and Temp =100-175 F

You may have to tweak the current densities and temperatures around
based on the complexity of your part.
hope it helps
Amrit.

On Mon, 15 Nov 2004 14:44:12 -0600, Charles Becnel  wrote:
> I am trying to electropolish 416 stainless steel.  Does anyone have a good
> procedure to accomplish this?
>
> Sincerely,
>
> Charles
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
>
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
Mentor Graphics Corporation
Nano-Master, Inc.
Tanner EDA by Mentor Graphics