Spin coating PDMS on wafer
Kevin Christ
2007-03-27
Peng,

I spin roughly 50 um thick membranes on 3 inch wafers at 1500 rpm for 15 sec.
My PDMS mixture, however, contains about 4% of Dow OS-20 methylsiloxane to make
spinning easier.

Kevin

-------------------------
Kevin V. Christ
Turner Research Group, http://ktgroup.me.wisc.edu
Department of Mechanical Engineering
University of Wisconsin, Madison
-------------------------

----- Original Message -----
From: "Peng Li (Paul)" 
Date: Monday, March 26, 2007 4:58 pm
Subject: [mems-talk] Spin coating PDMS on wafer
To: [email protected]

> Dear friends,
>
>  I want to spin coat PDMS on glass wafer to get 50um thickness layer.
> Does
>  anybody know where can I find data of PDMS thickness corresponding to
> spin speed?
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Tanner EDA by Mentor Graphics
MEMS Technology Review
The Branford Group