AZ5214E in image reversal mode
2007-05-16
Yue Mun Pun, Jeffrey
2007-05-16
Bill Moffat
2007-05-18
Zhang Xiao Qiang
2007-05-16
Chris Park
2007-05-16
Yue Mun Pun, Jeffrey
AZ5214E in image reversal mode
Chris Park
2007-05-16
Hi Jeffrey
I had the same experience with most of negative resist. They are very
sensitive to the PEB bake temp and time and exposure dose in stepper. If
you have good track and stepper, they are manageable. But if you have
some particle on hot plates and so on, you can lose your control fast.
Have you tried positive resist lift-off pattern by soaking on MF
developer before exposure?
Chris


-----Original Message-----
From: [email protected]
[mailto:[email protected]] On Behalf Of Yue Mun Pun, Jeffrey
Sent: Wednesday, May 16, 2007 2:39 AM
To: [email protected]
Subject: [mems-talk] AZ5214E in image reversal mode

Hi,
I have tried to use AZ5214E in image reversal mode to pattern some
alignment marks by lift-off process.  I have compared the image reversal
mode versus the positive imaging mode and found that the lift-off
process using image reversal is much more difficult than the positive
image mode.

Can anyone advise me on this matter?

Here is my image reversal process:
1.  Coat SiO2 wafer with AZ5214E spun at 2500rpm.  This gave me a resist
of thickness 1.4-1.6um.
2.  Soft bake at 95'C for 120s on hot plate.
3.  Expose at 405nm near UV light with intensity of about 7.5mW/cm2 for
5.4s to obtain average energy of 40mJ/cm2.
4.  Reversal bake on hot plate at 115'C for 120s.
5.  Flood expose at 405nm with intensity of 7.5mW/cm2 for 160s to obtain
average energy of 1200mJ/cm2.
6.  Develop in AZ400K developer diluted in DI water to a ratio of 1:4
for 45-60s.
7.  Thermal evaporation of 30nm Chromium.
8.  Lift off via both Acetone and PGMEA (SU-8 developer).

The wafer with the positive image was run as above except without the
reversal bake aqnd flood exposure.

Lift-off using the image reveral mode is very difficult even after
overnight soak in PGMEA.

Jeffrey
_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
The Branford Group
Addison Engineering
Process Variations in Microsystems Manufacturing