Ad Hall
2008-07-01
At the end of your CF4 etch switch to an O2 with 8% CF4 mixture and remove
around 20% of your resist.  Then remove the wafer from the RIE and wet
strip.

Ad Hall
StarCryoelectronics
505-424-6454
[email protected]


-----Original Message-----
From: [email protected] [mailto:[email protected]]
On Behalf Of Serena Eley
Sent: Tuesday, July 01, 2008 8:41 AM
To: [email protected]
Subject: [mems-talk] PR residue after CF4 RIE

Hi,

I used AZ5214 PR as a mask for CF4 RIE (47 sccm, 35mtorr, 90W).  I etched
for 6 min.  After removing the PR using nanoremover PG and IPA, there
remains about 10nm of residue that I can't remove.  I've tried hot
nanoremover, long sonication sessions in nanoremover, sonication in acetone,
DCM, O2 ash (300W, up to 10 min), and O2 RIE (20 sccm, 100W, up to 3 min).

Any suggestions for removing this residue? (Btw, I have a thin Ti capping
layer on Nb.  So, the residue is on oxidized Ti).

Thanks, Serena
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
University Wafer
The Branford Group
Mentor Graphics Corporation