MEMSnet Home: MEMS-Talk: Re: Cr/Au delamination
Re: Cr/Au delamination
2002-04-09
Jack Kotovsky
2002-04-09
Martin O. Patton
Re: Cr/Au delamination
Jack Kotovsky
2002-04-09
Hello Jiang;

I experienced similar difficulties and discovered my Au layer was
effectively porous and allowed HF (or other chemicals) to attack the Cr
adhesion layer.  Depending on your deposition technique/tool, you may find
a very thick (4000A in my case for our Ebeam evaporator) layer of Au is
required to fully protect your Cr.  I would recommend increasing your Au
thickness if possible or optimize your Au layer by optimizing the
deposition parameters for your dep tool or consider an alternate
application method (i.e. I would suspect electroplated Au would provide an
improved barrier to chemicals).

Best of luck, Jack

Jack Kotovsky
UC Davis Knee Orthopedics Laboratory


 > Date: Tue, 9 Apr 2002 08:39:45 -0700 (PDT)
> From: Jiang Zhe 
> To: [email protected]
> Subject: [mems-talk] Cr/Au delamination
> Reply-To: [email protected]
>
> I have a 300A Cr/2500A Au delamination problem. Cr/Au
>
> was deposited on p-type Si <100> wafer. Then it was
> put
>
> into concentrated HF and Cr/Au layer were peeled off
>
> after 30 minutes. The pre-clean (RCA clean and a 2min
>
> Ar plasma pre-etch) was well done before sputtering.
>
> My question is, what's the possible reason of the
>
> delamination? Any suggestion? Thanks!
>
> Jiang
> Yahoo! Tax Center - online filing with TurboTax
> http://taxes.yahoo.com/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Process Variations in Microsystems Manufacturing
Harrick Plasma, Inc.
Addison Engineering