MEMSnet Home: MEMS-Talk: Alternative to wet etching for glass
Alternative to wet etching for glass
2003-03-13
Haigh, Richard
2003-03-13
sp
2003-03-17
Michele Finardi
2003-03-19
Haigh, Richard
Alternative to wet etching for glass
Haigh, Richard
2003-03-19
Jamie

I am not too familiar with optical wave guide technology. As I understand it the
wave guide grooves must have a flat surface. The surface finish on a powder
blasted surface has a roughness of about 2 um. I am not too sure if this would
be too rough for your application


Richard

-----Original Message-----
From: Michele Finardi [mailto:[email protected]]
Sent: 17 March 2003 10:59
To: [email protected]
Subject: RE: [mems-talk] Alternative to wet etching for glass

Hallo Jamie,
do you know which is the quality of the vertical
facets after ultrasonic milling the powder blasting?
Do they have an optical quality (i.e.: is that a
technique that can be used for optical guides
manufacturing?)
Thank you.

Michele


-----Original Message-----
From: sp [mailto:[email protected]]
Sent: giovedì 13 marzo 2003 18.01
To: General MEMS discussion
Subject: Re: [mems-talk] Alternative to wet etching
for glass


Jamie,

You might also try ultrasonic milling for deep etching
in glass. Give us a
call
we provide ultrasonic milling services.

Steve Pence
408-980-9324

----- Original Message -----
From: "Haigh, Richard" 
To: "General MEMS discussion" 
Sent: Thursday, March 13, 2003 6:53 AM
Subject: [mems-talk] Alternative to wet etching for
glass


Jamie

An alternative route to wet etching that you might try
is powder
blasting. This is particularly suited to the abrason
of brittile
materials such as glass. Etch depths of 0.5 to 1 mm
can been achieved. A
Limiting factor is the appature width which is
typically no less than 70
um.

 Regards

Richard
-----Original Message-----
From: Zhimin J Yao [mailto:[email protected]]
Sent: 11 March 2003 19:59
To: [email protected]
Subject: [mems-talk] mask material for wet etch glass

Hi,

We are trying to etch about 0.5 - 1mm deep into glass
or quartz using a
metal mask.  Au did not work well because the adhesion
layer got etched.
Does anybody know what metal works the best?  Anybody
tried W?

Thanks,
Z. Jamie Yao


_______________________________________________
[email protected] mailing list: to unsubscribe or
change your list
options, visit
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS
processing services.
Visit us at http://www.memsnet.org/

_______________________________________________
[email protected] mailing list: to unsubscribe or
change your list
options, visit
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS
processing services.
Visit us at http://www.memsnet.org/




_______________________________________________
[email protected] mailing list: to unsubscribe or
change your list
options, visit
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS
processing services.
Visit us at http://www.memsnet.org/


______________________________________________________________________
Yahoo! Cellulari: loghi, suonerie, picture message per il tuo telefonino
http://it.yahoo.com/mail_it/foot/?http://it.mobile.yahoo.com/index2002.html

_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
MEMS Technology Review
The Branford Group
Process Variations in Microsystems Manufacturing