Property↑↓Value↑↓Conditions↑↓Reference↑↓
Density2197.7 kg/m^3Stabilized SiO2,Glass,at room temperature.CRC Materials Science and Engineering Handbook, p.53
Density2201 .. 2211 kg/m^3Glass,at room temperatureCRC Materials Science and Engineering Handbook, p.53
Electrical resistivity1e+16 Ω*mCeramic,at room temperatureCRC Materials Science and Engineering Handbook, p.566
Hardness,Knoop(KH)710 kg/mm/mm100g,Ceramic,parallel to optical axisCRC Materials Science and Engineering Handbook, p.474
Hardness,Knoop(KH)790 kg/mm/mm100g,Ceramic,normal to optical axisCRC Materials Science and Engineering Handbook, p.474
Hardness,Vickers(VH)1260 kg/mm/mm500g,Ceramic,parallel to optical axisCRC Materials Science and Engineering Handbook, p.474
Hardness,Vickers(VH)1103 kg/mm/mm500g,Ceramic,normal to optical axisCRC Materials Science and Engineering Handbook, p.474
Hardness,Vickers(VH)1120 kg/mm/mm500g,CeramicCRC Materials Science and Engineering Handbook, p.474
Thermal conductivity1.04 W/m/KCeramic,at temp=200 C.CRC Materials Science and Engineering Handbook, p.284
Thermal conductivity1.25 W/m/KCeramic,at temp=400 C.CRC Materials Science and Engineering Handbook, p.284
Thermal conductivity1.67 W/m/KCeramic,at temp=800 C.CRC Materials Science and Engineering Handbook, p.284
Thermal conductivity2.09 W/m/KCeramic,at temp=1200 C.CRC Materials Science and Engineering Handbook, p.284
Thermal conductivity2.51 W/m/KCeramic,at temp=1600 C.CRC Materials Science and Engineering Handbook, p.284
Thermal conductivity1.38 W/m/KGlass,at temp=20 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity0.59 W/m/KGlass at temp=80 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity0.67 W/m/KGlass,at temp=100 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity0.88 W/m/KGlass,at temp=150 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity1.28 W/m/KGlass at temp=250 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity1.32 W/m/KGlass,at temp=273.1 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity1.36 W/m/KGlass,at temp=300 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity1.43 W/m/KGlass,at temp=350 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity1.5 W/m/KGlass at temp=400 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity1.62 W/m/KGlass,at temp=500 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity1.72 W/m/KGlass,at temp=600 C.CRC Materials Science and Engineering Handbook, p.289
Thermal conductivity1.8 W/m/KGlass,at temp=700 C.CRC Materials Science and Engineering Handbook, p.289