| Property | Value | Conditions | Reference |
|---|
| Compressive strength | 0.2345 GPa | Ceramic,parallel to c axis | CRC Materials Science and Engineering Handbook, p.419 |
| Compressive strength | 0.3103 GPa | Ceramic,parallel to a axis | CRC Materials Science and Engineering Handbook, p.419 |
| Density | 3490 kg/m^3 | cubic | CRC Materials Science and Engineering Handbook, p.50 |
| Density | 3490 kg/m^3 | cubic | CRC Materials Science and Engineering Handbook, p.50 |
| Density | 2270 kg/m^3 | Hexagonal,Ceramic. | CRC Materials Science and Engineering Handbook, p.50-52 |
| Electrical resistivity | 1.7e+11 Ω*m | Ceramic,at temp=25 C | CRC Materials Science and Engineering Handbook, p.565 |
| Electrical resistivity | 2.3e+08 Ω*m | Ceramic,at temp=480 C | CRC Materials Science and Engineering Handbook, p.565 |
| Electrical resistivity | 310 Ω*m | Ceramic,at temp=1000 C | CRC Materials Science and Engineering Handbook, p.565 |
| Modulus of Rupture | 0.05021 .. 0.09103 GPa | Ceramic,parallel to c axis, at temp=25 C | CRC Materials Science and Engineering Handbook, p.533 |
| Modulus of Rupture | 0.04848 GPa | Ceramic,parallel to c axis, at temp=300 C | CRC Materials Science and Engineering Handbook, p.533 |
| Modulus of Rupture | 0.0131 GPa | Ceramic,parallel to c axis, at temp=700 C | CRC Materials Science and Engineering Handbook, p.533 |
| Modulus of Rupture | 0.007448 GPa | Ceramic,parallel to c axis, at temp=1000 C | CRC Materials Science and Engineering Handbook, p.533 |
| Modulus of Rupture | 0.008621 GPa | Ceramic,parallel to c axis, at temp=1500 C | CRC Materials Science and Engineering Handbook, p.533 |
| Modulus of Rupture | 0.010342 GPa | Ceramic,parallel to c axis, at temp=1800 C | CRC Materials Science and Engineering Handbook, p.533 |
| Modulus of Rupture | 0.0169 GPa | Ceramic,parallel to c axis, at temp=2000 C | CRC Materials Science and Engineering Handbook, p.533 |
| Modulus of Rupture | 0.1095 GPa | Cermic,parallel to a axis, at temp=25 C | CRC Materials Science and Engineering Handbook, p.533 |
| Modulus of Rupture | 0.1044 GPa | Ceramic,parallel to a axis, at temp=300 C | CRC Materials Science and Engineering Handbook, p.533 |
| Modulus of Rupture | 0.02648 GPa | Ceramic,parallel to a axis, at temp=700 C | CRC Materials Science and Engineering Handbook, p.533 |
| Modulus of Rupture | 0.01503 GPa | Ceramic,parallel to a axis, at temp=1000 C | CRC Materials Science and Engineering Handbook, p.533 |
| Tensile strength | 0.002413 GPa | Ceramic,at temp=1000 C | CRC Materials Science and Engineering Handbook, p.405 |
| Tensile strength | 0.002413 GPa | Ceramic,at temp=1500 C | CRC Materials Science and Engineering Handbook, p.405 |
| Tensile strength | 0.007931 GPa | Ceramic,at temp=1800 C | CRC Materials Science and Engineering Handbook, p.405 |
| Tensile strength | 0.01551 GPa | Ceramic,at temp=2000 C | CRC Materials Science and Engineering Handbook, p.405 |
| Tensile strength | 0.0469 GPa | Ceramic,at temp=2400 C | CRC Materials Science and Engineering Handbook, p.405 |
| Thermal conductivity | 28.72 W/m/K | Ceramic,parallel to c axis,at temp=300 C. | CRC Materials Science and Engineering Handbook, p.280 |
| Thermal conductivity | 27 W/m/K | Ceramic,parallel to c axis,at temp=700 C. | CRC Materials Science and Engineering Handbook, p.280 |
| Thermal conductivity | 26.63 W/m/K | Ceramic,parallel t c axis,at temp=1000 C. | CRC Materials Science and Engineering Handbook, p.280 |
| Young's Modulus | 33.864 GPa | Ceramic,at temp=23 C,parallel to c axis | CRC Materials Science and Engineering Handbook, p.508 |
| Young's Modulus | 23.924 GPa | Ceramic,at temp=300 C,parallel to c axis | CRC Materials Science and Engineering Handbook, p.508 |
| Young's Modulus | 3.512 GPa | Ceramic,at temp=700 C,parallel to c axis | CRC Materials Science and Engineering Handbook, p.508 |
| Young's Modulus | 85.945 GPa | Ceramic,at temp=23 C,parallel to a axis | CRC Materials Science and Engineering Handbook, p.508 |
| Young's Modulus | 10.606 GPa | Ceramic,at temp=700 C,parallel to a axis | CRC Materials Science and Engineering Handbook, p.508 |
| Young's Modulus | 11.367 GPa | Ceramic,at temp=1000 C,parallel to a axis | CRC Materials Science and Engineering Handbook, p.508 |