Property↑↓Value↑↓Conditions↑↓Reference↑↓
Compressive strength0.5517 .. 1.3103 GPaCeramic,at temp=25 CCRC Materials Science and Engineering Handbook, p.421
Density3160 .. 3220 kg/m^3Theoritical value,CeramicCRC Materials Science and Engineering Handbook, p.50-52
Density2600 .. 3260 kg/m^3CeramicCRC Materials Science and Engineering Handbook, p.50-52
Electrical resistivity1e+08 Ω*mCeramic,at temp=300 CCRC Materials Science and Engineering Handbook, p.567
Electrical resistivity1e+06 Ω*mAt temp=500 CCRC Materials Science and Engineering Handbook, p.567
Hardness,Vickers(VH)1120 kg/mm/mmCeramicCRC Materials Science and Engineering Handbook, p.474
Modulus of Rupture1232.5 GPaCeramic,density=2770 kg/m/m/m,temp=25 CCRC Materials Science and Engineering Handbook, p.535
Modulus of Rupture0.05862 GPaCeramic,density=2770 kg/m/m/m,temp=25 C.CRC Materials Science and Engineering Handbook, p.535
Modulus of Rupture0.04138 .. 0.1862 GPaCeramic,at temp=25 CCRC Materials Science and Engineering Handbook, p.535
Modulus of Rupture0.0931 GPaCeramic,density=2770 kg/m/m/m,at temp=400 CCRC Materials Science and Engineering Handbook, p.535
Modulus of Rupture0.1152 GPaCeramic,density=2770 kg/m/m/m,at temp=800 CCRC Materials Science and Engineering Handbook, p.535
Modulus of Rupture0.07931 GPaCeramic,density=2770 kg/m/m/m,at temp=1200 CCRC Materials Science and Engineering Handbook, p.535
Poisson's Ratio0.238Ceramic,density=2779 kg/m/m/mCRC Materials Science and Engineering Handbook, p.539
Tensile strength0.1103 GPaCeramic,at temp=25 CCRC Materials Science and Engineering Handbook, p.407
Thermal conductivity6.06 W/m/KCeramic,at temp=100 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.287
Thermal conductivity5.43 W/m/KCeramic,at temp=200 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.287
Thermal conductivity4.6 W/m/KCeramic,at temp=400 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.287
Thermal conductivity4.18 W/m/KCeramic,at temp=600 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.287
Thermal conductivity3.97 W/m/KCeramic,at temp=800 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.287
Thermal conductivity3.76 W/m/KCeramic,at temp=1000 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.287
Thermal conductivity3.76 W/m/KCeramic,at temp=1200 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.287
Thermal conductivity3.76 W/m/KCeramic,at temp=1400 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.287
Young's Modulus127.04 GPaCeramic,at temp=25 C,density=2770 kg/m/m/mCRC Materials Science and Engineering Handbook, p.511
Young's Modulus143.12 GPaCeramic,at room temperature ,density=2779 kg/m/m/mCRC Materials Science and Engineering Handbook, p.511
Young's Modulus130.27 GPaCeramic,at temp=400 C ,density=2770 kg/m/m/mCRC Materials Science and Engineering Handbook, p.511
Young's Modulus130.27 GPaCeramic,at temp=400 C ,density=2770 kg/m/m/mCRC Materials Science and Engineering Handbook, p.511
Young's Modulus102.02 GPaCeramic,at temp=800 C ,density=2770 kg/m/m/mCRC Materials Science and Engineering Handbook, p.511
Young's Modulus27.587 GPaCeramic,at temp=1200 C ,density=2770 kg/m/m/mCRC Materials Science and Engineering Handbook, p.511
Young's Modulus230.01 GPaCeramic,at room temperature ,full densityCRC Materials Science and Engineering Handbook, p.511