Property↑↓Value↑↓Conditions↑↓Reference↑↓
Compressive strength0.3241 .. 0.669 GPaCeramicCRC Materials Science and Engineering Handbook, p.419
Density4500 .. 4620 kg/m^3CeramicCRC Materials Science and Engineering Handbook, p.50
Electrical resistivity26.5 .. 284000 Ω*mCeramic,polycrystalline,85% dense,at room temperatureCRC Materials Science and Engineering Handbook, p.563
Electrical resistivity90000 Ω*mCeramic,polycrystalline,85% dense,at room temperatureCRC Materials Science and Engineering Handbook, p.563
Electrical resistivity8.7 .. 141000 Ω*mCeramic,polycrystalline,100% dense,at room temperature,extrapolated valuesCRC Materials Science and Engineering Handbook, p.563
Electrical resistivity37000 Ω*mCeramic,polycrystalline,100% dense,at liquid air temperature, extrapolated valuesCRC Materials Science and Engineering Handbook, p.563
Electrical resistivity64000 .. 68000 Ω*mCeramic,monocrystalline,crystal length 5 cm,39 deg.and 59 deg.orientation with respect to growth axis,at room temperatureCRC Materials Science and Engineering Handbook, p.563
Electrical resistivity6.5e+06 .. 6.9e+06 Ω*mCeramic,monocrystalline,crystal length 1.5 cm,16.5 deg.and 90 deg. orientation with respect to growth axis,at room temperatureCRC Materials Science and Engineering Handbook, p.563
Hardness,Knoop(KH)3370 kg/mm/mmCeramic,30gCRC Materials Science and Engineering Handbook, p.470
Hardness,Knoop(KH)2710 .. 3000 kg/mm/mmCeramic,100gCRC Materials Science and Engineering Handbook, p.470
Hardness,Knoop(KH)3500 kg/mm/mmCeramic,160gCRC Materials Science and Engineering Handbook, p.470
Hardness,Vickers(VH)3400 kg/mm/mmCeramic,50gCRC Materials Science and Engineering Handbook, p.470
Modulus of Rupture0.132 GPaCeramicCRC Materials Science and Engineering Handbook, p.532
Modulus of Rupture0.03703 GPaCeramic,98% denseCRC Materials Science and Engineering Handbook, p.532
Poisson's Ratio0.09 .. 0.28CeramicCRC Materials Science and Engineering Handbook, p.537
Tensile strength0.1269 GPaCeramicCRC Materials Science and Engineering Handbook, p.405
Thermal conductivity24.24 .. 25.92 W/m/KAt room temperature.CRC Materials Science and Engineering Handbook, p.278
Thermal conductivity26.33 W/m/KAt temp=200 C.CRC Materials Science and Engineering Handbook, p.278
Young's Modulus366.9 GPaCeramicCRC Materials Science and Engineering Handbook, p.507