Property↑↓Value↑↓Conditions↑↓Reference↑↓
Hardness,Knoop(KH) or Vickers(VH)713 .. 1121 kg/mm/mmCeramicCRC Materials Science and Engineering Handbook, p.474
Modulus of Rupture0.06897 .. 0.1028 GPaCeramic,at room temperatureCRC Materials Science and Engineering Handbook, p.535
Poisson's Ratio0.28CeramicCRC Materials Science and Engineering Handbook, p.538
Thermal conductivity6.69 W/m/KCeramic,at temp=100 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.284
Thermal conductivity5.02 W/m/KCeramic,at temp=200 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.284
Thermal conductivity3.76 W/m/KCeramic,at temp=400 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.284
Thermal conductivity3.34 W/m/KCeramic,at temp=600 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.285
Thermal conductivity3.34 W/m/KCeramic,at temp=800 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.285
Thermal conductivity3.34 W/m/KCeramic,at temp=1000 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.285
Thermal conductivity3.34 W/m/KCeramic,at temp=1200 C,porosity=0%.CRC Materials Science and Engineering Handbook, p.285
Young's Modulus282.76 GPaCeramicCRC Materials Science and Engineering Handbook, p.510