MEMSnet Home: MEMS-Talk: ITO Etch selective to glass
ITO Etch selective to glass
2004-02-23
Anthony
2004-02-23
Philip D. Floyd
2004-02-23
Bill Moffat
ITO Etch selective to glass
Philip D. Floyd
2004-02-23
Anthony,

To etch the ITO, HCl will work.  Data on HCl etching of ITO can be found
here:
http://www.betelco.com/sb/phd/ch5/c52.html



Commercial ITO Etchant
http://www.transene.com/tino.html

MSDS can be found
http://grover.mirc.gatech.edu/data/msds/406.html

This is made up of FeCl-HCl-H2O.  If you hunt around a bit, you should be
able to find the proportions of each etchant required.

Both etchants will leave SiO2 unetched, to my knowledge.

Good Luck,

************************************
Philip D. Floyd, Ph.D.
Iridigm Display Corporation
2415 Third Street, Suite 235
San Francisco, CA 94107
ph:  (415) 626-8800 x138
fax: (415) 626-9775
email: [email protected]
web:  http://www.iridigm.com/
*************************************
############################################################################
##############################################
This email communication may contain CONFIDENTIAL INFORMATION of IRIDIGM
DISPLAY CORPORATION and is intended only for the use of the intended
recipients identified above. If you are not the intended recipient of this
communication, you must not use, disclose, distribute, copy or print this
email. If you have received this communication in error, please immediately
notify the sender by reply email, delete the communication and destroy all
copies.
############################################################################
##############################################


-----Original Message-----
From: Anthony [mailto:[email protected]]
Sent: Monday, February 23, 2004 5:33 AM
To: [email protected]
Subject: [mems-talk] ITO Etch selective to glass

I am looking for an etch that will remove Indium Tin Oxide (ITO) on a glass
lens without damage to the lens.  The ITO will need to be patterned. What
would be the best approach to do this?

Anthony Marrs
Intellite
[email protected]



_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
University Wafer
Mentor Graphics Corporation
Process Variations in Microsystems Manufacturing