Mask against TMAH and KOH Etching
2004-05-01
[email protected]
2004-05-02
Ashwin
2004-05-03
Gert Eriksen
Mask against TMAH and KOH Etching
Gert Eriksen
2004-05-03
Dear Y.C. Lin,

I think that you have a problem with the silicon nitride. Both KOH and TMAH
should be
masked easily with 1500 A LPCVD silicon nitride. Check the refractive index. It
should be
somewhere around 2.05 to 2.10 ( I don't rememer the exact figures). Otherwise,
you could
have too many pinholes in the film.

As mask material you could use thermal grown silicon oxide instead. The
selectivity of
silicon to silicon oxide is around 100 for 30 wt.% KOH at 80C. In TMAH the
selectivity is
generally much higher (> 1000), but I don't know the exact figure for an 8 %
concentration. Low concentrations of TMAH gives rough surfaces, but high etch
rates. For
better surface quality, concentrations above 15% are preferred.

Regards,
Gert Eriksen




On 1 May 2004 at 22:37, [email protected] wrote:

> Dear all:
>
> I have questions about the TMAH and KOH etching.
> I use a layer of LPCVD nitride with 1500A thick.
> After 3 hours KOH etching (30% w.t., 80C), the nitride layer is etched
seriously.
> Similarly, the nitride layer cannot survive in TMAH (8% w.t., 90C) for more
than 5 hours.
> Is there any method or material that can be used as the etching mask in TMAH
and KOH for
> at least 11 hours? Please give me some advice. I really appreciate it.
>
> Regards,
>
> Y.C. Lin
>
> Dept. of Power Mechanical Engineering,  National Tsing Hua University, Taiwan.
>
>
>
>
>
>
>
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/




reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
Harrick Plasma, Inc.
The Branford Group
Process Variations in Microsystems Manufacturing