MEMSnet Home: MEMS-Talk: PMMA bonding
PMMA bonding
2004-10-28
Mielnik, Michal
2004-10-28
David Barrow
PMMA bonding
David Barrow
2004-10-28
Dear Michal
you can thermally bond the parts quite simply with an ordinary lab oven, pieces
of flat glass and weights as required. Apart from obvious cleanliness a key
trick to avoid large air pockets in the bond is to prebake the parts for ~90
degrees for up to 2 days (weekend is good).
David
-----------------------------------------------
Professor David Barrow
Laboratory for Applied Microsystems Cardiff School of Engineering
Cardiff University
Queen's Buildings
1-5 The Parade
PO Box 689
Cardiff CF24 3TF
Wales
United Kingdom
Tel   +44(0)29 2087 5921 (Office)
Tel   +44(0)29 2087 4716 (Laboratory)
Mob   +44(0)77 8526 4780
E-m   [email protected]
-----------------------------------------------

>>> [email protected] 28/10/04 4:27 PM >>>
Hello,

Can anybody suggest a simple method for bonding two pieces of PMMA together?
Basically a PMMA chip w/microchannels and a PMMA cover.
We don't have any fancy equipment, so the simpler, the better.
I'm considering thermal bonding.
For thermal bonding; what kind of temperatures? pressures? baking times? can I
just bake the thing in air atmosphere? Any cleaning considerations?
Maybe there are other methods that are more suitable (adhesives, solvents...)
I'm completely new to this, so any comments or suggestions would be greatly
appretiated.

Thanks.

regards,

Michal Mielnik
Norwegian University of Science and Technology (NTNU)
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
Nano-Master, Inc.
Process Variations in Microsystems Manufacturing
Tanner EDA by Mentor Graphics