MEMSnet Home: MEMS-Talk: anodic bonding: contaminants at glass top surface
Crosslink PMMA
2005-12-01
[email protected]
2005-12-02
Fabio Altomare
anodic bonding question
2005-12-02
Robert Dean
2005-12-03
Kirt Williams
anodic bonding: contaminants at glass top surface
2005-12-20
Antonius Helvoort
2005-12-21
Shay Kaplan
2005-12-21
Shile
2005-12-05
Brubaker Chad
anodic bonding: contaminants at glass top surface
Shay Kaplan
2005-12-21
Ton,
Use graphite on top of the glass
Shay

-----Original Message-----
From: [email protected] [mailto:[email protected]]
On Behalf Of Antonius Helvoort
Sent: Tuesday, December 20, 2005 7:14 PM
To: [email protected]
Subject: [mems-talk] anodic bonding: contaminants at glass top surface

Dear all,

When bonding sodium containing glasses, at the cathode side (top glass
surface) sodium hydroxide can form as a contaminant. This is thought to be
due to the reaction between the migrated sodium and moisture.

This effect could be avoided by chosing a different electrode geometry or
material. Can anyone give me ideas or references for avoiding this specific
problem.

Thanks in advance,
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Tanner EDA by Mentor Graphics
University Wafer
Process Variations in Microsystems Manufacturing