A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Hf resistant Adhesion layer for Au on Si
Hf resistant Adhesion layer for Au on Si
2008-04-03
Heiko Prüßner
2008-04-03
Morrison, Richard H., Jr.
2008-04-03
Ruiz, Marcos Daniel (SENCOE)
2008-04-03
Brent Garber
2008-04-04
Michael Larsson
2008-04-09
Heiko Prüßner
2008-04-09
Shay Kaplan
2008-04-09
Jesse D Fowler
Hf resistant Adhesion layer for Au on Si
Shay Kaplan
2008-04-09
Try to use Ti as adhesion layer.

Shay

-----Original Message-----
From: [email protected] [mailto:[email protected]]
On Behalf Of Heiko Pr??ner
Sent: Wednesday, April 09, 2008 1:23 PM
To: General MEMS discussion
Subject: Re: [mems-talk] Hf resistant Adhesion layer for Au on Si

Dear All,

thank you for your replies on my question about the adhesion problem of my
thermally treated Cr/Au layer (see below).

Your suggestion about the interdiffusion of Cr and Au seem to be correct. I
found out that the thermal step already destroys the adhesion of the films.
Also I tested some chips with 20nm Cr/ 200nm Ni / 200nm Au which I already
had here. They worked fine even for 3 hours at 380degC. So Ni as diffusion
barrier seem to work. Due to stress reasons 200nm Ni might be to thick for
my application. Does anyone know what minimum thickness for Ni as diffusion
barrier is necessary?
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
MEMStaff Inc.
MEMS Technology Review
Tanner EDA by Mentor Graphics