MEMSnet Home: MEMS-Talk: "cavity" formation after annealing of evaporated aluminium on Si
"cavity" formation after annealing of evaporated aluminium on Si
2008-09-26
Julie Verstraeten
2008-09-27
shay kaplan
2008-09-27
Bill Moffat
2008-09-29
Julie Verstraeten
2008-09-30
Ngo Ha Duong
"cavity" formation after annealing of evaporated aluminium on Si
Julie Verstraeten
2008-09-26
Hi everyone,

We currently have some problems with the deposition of aluminium layers.
Maybe some of you already experienced that phenomenon:

Some bump-like structures appear all over the sample after the annealing of
the evaporated Al layer (see second SEM picture). These structures seem to
be empty inside however this could be the effect of the cleave.

The test samples are bare silicon cleaned with solvents (opticlear, acetone
and IPA, 5min each with ultra-sound). They are then immersed in a solution
of 8% HF: DI to etch the native oxide (10-15sec until hydrophobicity) just
before evaporation. The aluminium is then evaporated (e-beam) at a rate of
0.3nm/sec (250nm).=20

The samples surface seems very clean before the evaporation. After
evaporation, the Al surface shows little protuberances (~100nm, see =
first SEM picture).

The 450=B0C annealing, during 30min, reveals the cavern-like structures
(~500nm-1=B5m).  The annealing was performed under N2 atmosphere and forming
gas (N2 80%, H2 20%); both lead to the same results.

We don=92t know if this comes from
- a cleaning problem (traces of water or solvent at the surface before
evaporation),
- some problem during evaporation  (contamination, non uniform deposition,
stresses) amplified during annealing,
- some contamination in the oven.


Does anyone have any advice or suggestions?

Aluminium on Si after evaporation (no annealing)

Evaporated Aluminium on Si after 30min annealing at 450=B0C

Thank you,

Julie
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Mentor Graphics Corporation
Process Variations in Microsystems Manufacturing
Addison Engineering