selective etching InGaAs to InP
Zhen Peng
2009-03-18
Try H2SO4:H2O2:H2O (3:1:1) at room temp. I do not have etch rates in hand,
but it should etch InGaAs very fast and almost no etching of InP.

Zhen

-----Original Message-----
From: weiquan yang [mailto:[email protected]]
Sent: Tuesday, March 17, 2009 1:30 PM
To: [email protected]
Subject: [mems-talk] selective etching InGaAs to InP

Hi, all. Do you know a wet InGaAs etchant with high selectivity to InP. I
etched InGaAs using InP as the mask. Because the InP is useful for our final
device, I looked for the solution with high selective etching InGaAs to
InP.The etching rate to InGaAs should be as big as possible, and the etching
rate to InP should be as small as possible. I tried HF+H2O2. the selectivity
is kind of OK, however it will react with SiO2, which is a useful layer in
our device. I  also tried  C6H8O7+H2O2. The etching rate to InGaAs is not
fast enough. Are there people who have experience in InGaAs and InP? Pls
give me some advice. Thanks a lot.


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Tanner EDA by Mentor Graphics
MEMS Technology Review
MEMStaff Inc.