A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: KOH and TMAH etch masks other than SiN for long Si etch
KOH and TMAH etch masks other than SiN for long Si etch
2009-04-21
l j
2009-04-21
Xiaoguang Liu
2009-04-21
Brian Stahl
2009-04-22
Yongliang Yang
KOH and TMAH etch masks other than SiN for long Si etch
2009-04-25
Chris P. Park
2009-04-22
Shao Guocheng
2009-04-22
Prem Pal
KOH and TMAH etch masks other than SiN for long Si etch
Chris P. Park
2009-04-25
Hi K.C,

under-etching of the hard mask is a typical problem with long KOH etching
processes as the adhesion of the masking material on the
bevelled wafer edges is poor. We have also seen the problem with HF-etching of
glass wafers with a polysilicon hard mask. We use a
mechanical wafer holder (from AMMT, www.ammt.com) that protects the edge of the
wafer to avoid this as we have not found any deposition
technique suitable for edge protection.

Best regards,

Chris.




----- Original Message ----
From: l j 
To: [email protected]
Sent: Tuesday, April 21, 2009 3:49:24 AM
Subject: [mems-talk] KOH and TMAH etch masks other than SiN for long Si etch

Hello MEMS community,

I am looking for input on problems with etch masking for long Si anisotropic
etch.
Recently I found myself needing to do anisotropic ~500 micron etch of Si (100)
wafers, both sides polished. I do not have silicon nitride available as an
option.

I have studied recipes for etch and masks. Seems like the prescription for mask
is CVD silicon nitride. For other mask options, recommendations seem to get less
certain and more sketchy.
Pulling together references I could find, I have tried KOH 50% 80C and TMAH 25%
80C. The etch itself works as expected on the Si (100).

For masking I have tried Ti 500A / Au 2500A sputtered at 300C; Cr 500A / Au
2500A sputtered at 300C; SiO2 500A sputtered at 300C. Wafers were solvent
cleaned and oxygen plasma cleaned prior to metal deposition.

For the metal masks, after an hour or two in etch, it appears the adhesion layer
Ti or Cr is being attacked, and with another hour or  two, the Au is almost
floating off the Si, intact but without the Ti or Cr.

For the SiO2 mask in the TMAH, it appears the TMAH got through the SiO2 mask
within an hour.
So, are Ti or Cr and Au known to work, or not, as etch mask for long KOH or TMAH
etch? Is there a solid reference in the literature? The behavior I saw reminds
me of a description of anodic dissolution (M. Datta, “Anodic dissolution of
metals at high rates,” IBM Journal of.. Research and Development, vol. 37, pp.
207–226, 1993.) I also found in memsnet a reference to the metal and Si
combination resulting in a "primary cell" which removes the adhesion layer, but
was a little sketch on details.

Is sputtered SiO2 not dense enough to mask TMAH? Si/SiO2 selectivity of TMAH is
supposed to be very high.

Look forward to any insights.
Thank you
K.C.

_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk





reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation
Harrick Plasma, Inc.
MEMStaff Inc.