MEMSnet Home: MEMS-Talk: Alignment problem with Multilayer SU-8 fabrication
Alignment problem with Multilayer SU-8 fabrication
2014-05-15
[email protected]
2014-05-14
Bill Chow
2014-05-14
Gareth Jenkins
2014-05-14
[email protected]
2014-05-16
Jiho Song
2014-05-16
Daniel Figura
2014-05-16
hamideh jafarpoor
2014-05-16
王舒禹
2014-05-16
Matthieu Nannini
2014-05-16
sangee vs
2014-05-19
[email protected]
Alignment problem with Multilayer SU-8 fabrication
[email protected]
2014-05-14
We had similar problems with a thick photoresist (9.7 um) due to trapped air
that would explode upon heating up the resist post-coat. What seemed to help the
most was to redesign the alignment marks - keep them narrow and short. The
second thing that helped was to let the PR settle for a few minutes after
spinning before exposing it to any kind of heat.

Hope this helps.

Regards,

-Deep






Sent from Windows Mail





From: Bill Chow
Sent: ‎Wednesday‎, ‎May‎ ‎14‎, ‎2014 ‎9‎:‎14‎ ‎AM
To: General MEMS discussion





Dear all,

Recently, I am working on a two layer SU-8 structure. All the process are
followed with the suggested procedures. However, the problem appeared when I
try to look for the alignment mark, after I have spin coated and prebaked
the second layer of SU-8, it is difficult to locate the first layer exposed
features.

First layer thickness : 3.7um
Second layer thickness : 17 - 20um

I found that it is extremely difficult to locate the first layer pattern
under the microscope after I have coated the second layer, despite it can be
seen be naked eye.... Sometimes if there are some defect or bump in the 2nd
layer above the alignment mark, then it can be seen clearly. However, it  is
a random process and will affect my pattern. Are there any ways to improve
the visiblity of the alignment mark after I have coated the 2nd layer?
Thanks.

Regards,

Bill

_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Mentor Graphics Corporation
MEMS Technology Review
Tanner EDA by Mentor Graphics
Process Variations in Microsystems Manufacturing