MEMSnet Home: MEMS-Talk: About difficulty in photoresist development (if using HMDS as adhesion layer)
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-23
Mehmet Yilmaz
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-24
Bill Moffat
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-24
André Bödecker
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-24
James Guenes
2015-09-25
Liang Zhao
2015-09-25
Orozaliev Ajymurat Nurdinovich
2015-09-29
Mehmet Yilmaz
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-25
Mohammad Yusuf Mulla
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-29
Andrew Sarangan
2015-09-30
Mehmet Yilmaz
2015-10-04
Andrew Sarangan
2016-01-04
Mehmet Yilmaz
2016-01-04
조명래
2016-01-04
ozgur celik
2016-01-05
André Bödecker
2015-09-25
Brian Baker
About difficulty in photoresist development (if using HMDS as adhesion layer)
Orozaliev Ajymurat Nurdinovich
2015-09-25
Mehmet,

HMDS shouldn't have an effect on development time since it is only a single
layer.
I would check the baking temperature and time.
Also, if you are using the YES oven, try to coat the resist after the wafer
temperature reduces to room temperature.

I sometimes do not use HMDS at all. Instead I bake the wafer at 200 C for 5
mins and after it cools down I immediately coat my resist and I do not have
an adhesion problem.

good luck,
Ajy



On Thu, Sep 24, 2015 at 4:21 PM, James Guenes  wrote:

> Mehmet,
> your problem is the combination of thickness combined with HDMS.
>
> Potential Solution:
> Have a list of the properties of the HDMS and find a compound that will not
> insist to stick to the matter for a very long time, which means you have to
> conduct experiments with various solutions under tightly controlled
> environments.
>
> All the best of luck to you, I hope that my observation was a little
> insightful,
>
> On Mon, Sep 21, 2015 at 5:24 AM, Mehmet Yilmaz 
> wrote:
>
> > Dear mems-talk community,
> > If I use HMDS as adhesion layer, I am having a problem with the
> development
> > of a photoresist called AZ4562 (about 10 micron thickness). In addition,
> I
> > am having the same development problem with AZ5214E (about 1.4 micron
> > thickness).
> >
> > If I do not use HMDS, the development time is usually about 60 seconds,
> or
> > even less. However, if I use HMDS, the development time goes up to 45
> > minutes (not seconds...) and still the development is not successful, but
> > the resist is completely removed from some parts of the patterned areas
> on
> > the wafer.
> >
> > Also, I have seen this problem with different substrates such as Silicon,
> > Quartz, and Pyrex.
> >
> > I am wondering what would be the reason for that? Is it possible that
> HMDS
> > is old, and out of date? Could that explain the problem? Or, do you have
> > any other comments based on your own experience? Could you please
> comment?
> >
> > I am looking forward to your replies.
> >
> > Thanks in advance,
> >
> > Mehmet
> >
> > Mechanical Engineer
> > _______________________________________________
> > Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> > provider of MEMS and Nanotechnology design and fabrication services.
> > Visit us at http://www.mems-exchange.org
> >
> > Want to advertise to this community?  See http://www.memsnet.org
> >
> > To unsubscribe:
> > http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> >
>
>
>
> --
> James Guenes
> Electrical, Controls, Integration, Automation, Systems, Research, Reverse,
> and Process Engineer
> 513.482.9175 cell
> Connect With Me on LinkedIn
> <
> https://www.linkedin.com/profile/public-profile-settings?trk=prof-edit-edit-
public_profile
> >
> ------------------------------
> *The information in this email is intended only for the personal and
> confidential use of the designated recipient above. If the reader of this
> message is not the intended recipient or an agent responsible for
> delivering it to the intended recipient, you are hereby notified that you
> have received this document in error, and that any review, dissemination,
> distribution or copying of the message is strictly prohibited. If you are
> not the intended recipient, please contact the sender immediately by reply
> e-mail and destroy all copies of the original message.*
> _______________________________________________
> Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> provider of MEMS and Nanotechnology design and fabrication services.
> Visit us at http://www.mems-exchange.org
>
> Want to advertise to this community?  See http://www.memsnet.org
>
> To unsubscribe:
> http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>
_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
University Wafer
Process Variations in Microsystems Manufacturing
Harrick Plasma, Inc.