MEMSnet Home: MEMS-Talk: Lift-off of AZ5214
Lift-off of AZ5214
2002-03-08
Peng Yao
2002-03-11
Bill Moffat
2002-03-12
Biao Li
Lift-off of AZ5214
Biao Li
2002-03-12
Hi, Bill,

I got the reversal image using AZ5214 with a different way: coating,
prebaking, exposure, baking, flood exposure, and develop. No ammonia is used
in my case. And I always illuminate the phororesist for 60sec or more during
the flood exposure. Do you have any data or literature about the effect of
flood exposure on the angle of overhang? In my opinion, this angle is
determined mainly by the exposure and develop time.

Thanks a lot.

Biao Li
Albany nanoTech

-----Original Message-----
From: Bill Moffat [mailto:[email protected]]
Sent: Monday, March 11, 2002 11:10 AM
To: [email protected]
Subject: RE: [mems-talk] Lift-off of AZ5214


Peng,
     One way to get a negative angle is to use an image reversal technique.
My company manufacture a reversal unit which uses ammonia.  In principle you
do the first exposure which determines the C.D. then place in ammonia at 90
degrees centigrade for 45 minutes.  The ammonia neutralizes the acid in the
exposed areas.  Then flood expose which determines the angle of overhang.  I
have numerous technical papers on the subject as there are hundreds of units
in operation.  Typical C.D. would be 0.1 micron. typical overhang up to 22
degrees reverse angle.  Once the C.D. is established with the first exposure
the flood exposure controls the angle of the resist can be controlled from
22
degrees either side of vertical.  People looking for extreme resolution use
vertical side walls.  Bill Moffat

-----Original Message-----
From: Peng Yao [mailto:[email protected]]
Sent: Friday, March 08, 2002 11:44 AM
To: [email protected]
Subject: [mems-talk] Lift-off of AZ5214


Hi,
The result of lift off is determined by the profile of your side wall of
PR structures after development. I usually use negative photoresist to get
the negtive angel I want. And for that, lift off is very easy.
According to the book "fundamentals of microfabrication", it was said if
you control the exposure and develop time, you can get both negative and
positive side wall, but I never succeeded in the former one. I am also
very interested in this topic. If anyone can make a negative side wall
using AZ5214?


Peng Yao
DOEs lab
Electrical Engineering Dept.
Univeristy of delaware
Newark D.E 19716
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
Tanner EDA by Mentor Graphics
Addison Engineering
The Branford Group