Dear Glen,

I've worked pretty extensively, and have noticed this phenomenon as well.
In my opinion, the following items helped to resolve this issue:

1 -     Use of high acceleration to ramp up to spin off speed.  I know that
this is contrary to what some others on the group have said, but the
principle of the high spin off makes sense.  The reason for the "starfish"
pattern has more to do with the surface tension of the resist than of its
viscosity.  Basically, once a "tendril" of resist has made it to the edge of
the wafer, the path of least resistance for the flow of resist is within
that "tendril", since the surface tension of the walls of the "tendril" is
so high.

By using high acceleration (>10,000 rpm/sec, ideally), there is a greater
amount of force present to draw the resist outwards on the wafer.
Additionally, the rapid acceleration motion breaks up the surface, allowing
smoother flow.
2 -     As one reader mentioned, the use of a cover for the coater bowl will
also help more even spreading of the resist.  Again, this is an attempt to
reduce surface tension, this time by preventing drying of the outer surface
of the resist.  Because of the very high solids content (~70%), evaporation
of solvent causes a very rapid increase of viscosity at the surface of the
resist, and with an increase of viscosity comes an increase surface tension.
The use of a cover traps evaporating solvent, and greatly reduces drying.
In addition to allowing a better spread of resist, the use of a cover will
improve resist uniformity as well.

Best Regards,
Chad Brubaker


EV Group-Technology, Tel: (602) 437 9492 x 119, Fax: (602) 437 9435
E-mail: [email protected],  Web: www.EVGroup.com, 03/15/02

-----Original Message-----
From:   Glen Landry [mailto:[email protected]]
Sent:   Friday, March 15, 2002 6:24 AM
To:     [email protected]
Subject:        [mems-talk] SU-8 spinning problems

I have a problem spinning SU-8 2050 photoresist (Microchem corp). When
I place the required amount on my 2" silicon wafer and spin, it does not
spread uniformly. Instead it all goes to one side (if it is not exactly
centered) or it spreads out in a starfish pattern, leaving large portions
of the wafer uncovered.
I have tried manually spreading the SU-8 across the wafer, with my
pipette, but this introduces bubbles. It was also suggested to tilt the
wafer to get the SU-8 to spread, or to sit it on a table. Neither of these
suggestions worked, since the SU-8 2050 is so viscous and it takes so long
to spread with gravity, a skin forms on the SU-8 before it spreads.

Does anyone have suggestions?
Glen Landry
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
MEMStaff Inc.
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation