MEMSnet Home: MEMS-Talk: RE: RE: [mems-talk] How to clean Si wafer with Cr/Au before anodic bo nding
How to clean Si wafer with Cr/Au before anodic bo nding
2002-09-30
[email protected]
RE: RE: [mems-talk] How to clean Si wafer with Cr/Au before anodic bo nding
2002-10-01
Phyllis Yuen
RE: RE: [mems-talk] How to clean Si wafer with Cr/Au before anodic bo nding
Phyllis Yuen
2002-10-01
The Au layer act as a mirror so roughening it might defect the purpose.
Will oxygen plasma clean be good enough for anodic bonding?
Thank you for your help!
Phyllis Yuen
UC Davis
 [email protected] wrote: > I would like to bond Si and pyrex wafer
together by anodic
> bonding. My Si wafer has some trenches which the bottom is
> covered by a 200A Cr/ 500A Au. How can I clean this Si wafer
> before anodic bonding? Can I do RCA SC1 clean
> (water+H2O2+Ammonia solution) to remove organic
> contaminations, without the RCA SC2 clean (water+H2O2+HCl),
> which remove the metallic contaminations?

You can do a Piranha clean (H2SO4 + H2O2, 120 C) for 5 minutes.
In our experiments with different gold samples (with chromium adhesion layer),
one was not etched at all and the other was roughened slightly.

--Kirt Williams Agilent Technologies




---------------------------------
Do you Yahoo!?
New DSL Internet Access from SBC & Yahoo!
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Addison Engineering
Nano-Master, Inc.
The Branford Group