Niobium dry etching
[email protected]
2002-04-19
We have had some experience of etching Niobium layers, too.  We also used
SF6, but in an ICP system.  This gave an undercut profile initially.  Adding
oxygen helped to passivate the sidewalls (but would not be good for
photoresist selectivity).  We were using hard (PECVD SiO2) masking.  The
etch rate was around 150nm/min.

Martin Walker, Oxford Instruments

>Roger Shile [email protected]
>Thu, 18 Apr 2002 09:18:12 -07
>I have had success etching Nb with pure SF6 plasma using a March Jupiter
RIE
>system.  The electrode diameter was ~ 6".  RF power was 50 watts.  Pressure
>wass 200 mTorr (?).
>
>1.3 microns of hard-baked resist was more than adequate as a mask to etch
4000
>Angstroms Nb films.
>
>Roger Shile
>
>>> [email protected] 04/18/02 03:34AM >>>
>Hi all,
>
>I have been trying to etch Niobium using CF4 plasma but the process seems
more
>willing to strip
>the photoresist before it etches into the metal. Does CF4 have problems
with
>selectivity or is there
>another recipe for this process that could be used.
>
>Mike


 ###  OXFORD INSTRUMENTS   http://www.oxford-instruments.com/  ###

Unless stated above to be non-confidential, this E-mail and any
attachments are private and confidential and are for the addressee
only and may not be used, copied or disclosed save to the addressee.
If you have received this E-mail in error please notify us upon receipt
and delete it from your records. Internet communications are not secure
and Oxford Instruments is not responsible for their abuse by third
parties nor for any alteration or corruption in transmission.

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation
Tanner EDA by Mentor Graphics
The Branford Group