MEMSnet Home: MEMS-Talk: wet etch recipe for Iridium (Ir)
wet etch recipe for Iridium (Ir)
2007-01-28
Mantavya <Manu> Sinha
2007-01-29
David Nemeth
2007-02-11
Mantavya Sinha
2007-02-21
Mantavya Sinha
2007-02-22
David Nemeth
2007-01-29
Mantavya Sinha
wet etch recipe for Iridium (Ir)
David Nemeth
2007-02-22
Manu,
  Perhaps your best bet is to give up on etching and try a liftoff, if that
works with you process.  Or use an ion mill.  Some things are too hard to
etch chemically.

David Nemeth

-----Original Message-----
From: [email protected] [mailto:[email protected]]
On Behalf Of Mantavya Sinha
Sent: Tuesday, February 20, 2007 10:48 PM
To: General MEMS discussion
Subject: RE: [mems-talk] wet etch recipe for Iridium (Ir)

Thanks for the help David. Unfortunately, it still doesn't seem to work.
I tried hot(85'C) un-diluted aqua regia (3 parts HCL, 1 part HNO3) for
as long as 30mins and I had only 15nm of Ir and still there was no
etching.
I also tried another recipe (1part HNO3 + 5 part H2O + 10part HCl at
85'C) but didn't get any results.

Does anyone have any experience in wet etching Iridium? Any pointers
would be highly appreciated.

Regards,
Manu
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
Addison Engineering
Process Variations in Microsystems Manufacturing
MEMStaff Inc.