MEMSnet Home: MEMS-Talk: AZ9260 double spinning recipe
AZ9260 double spinning recipe
2013-10-03
Orozaliev Ajymurat Nurdinovich
2013-10-03
basar bolukbas
2013-10-03
Jonathan Lueke
2013-10-06
Orozaliev Ajymurat Nurdinovich
2013-10-03
Gary Hillman
2013-10-04
Alex Feldman
2013-10-04
Ioannis Nikolaou
2013-10-04
Orozaliev Ajymurat Nurdinovich
2013-10-06
Ioannis Nikolaou
AZ9260 double spinning recipe
Jonathan Lueke
2013-10-03
I use AZ4620 for a similar etch. 2 layers. About 25-26um.

Two questions:

1. Do you allow for a full rehydrate between depositions of resist?

2. Have you tried a longer hard bake? 10-15 min?

Our processes are very similar except those two steps.

Jon

----------------------------
Jonathan Lueke B.Sc., E.I.T.
Ph.D. Candidate
Department of Mechanical Engineering
University of Alberta
(780)6906468

Sent from my iPhone

On 2013-10-03, at 1:30 AM, Orozaliev Ajymurat Nurdinovich 
wrote:

> Hi All,
>
> I was working on thick AZ9260 resist for using as a mask on DRIE tool.
> My target is to etch 450-480 um of Silicon. I have preliminary results for
> PR:Si selectivity, which is ~1:25. To etch 450 um of Si, I would need at
> least 18 um(but more the better) of AZ9260. With single coating I am
> getting maximum of 15 um. But when I do double spinning and expose it, the
> resist is turning yellowish-orange. Further, I develope it, but when I put
> it inside the DRIE tool, after a few cycles, the resist is forming flakes
> and contaminating inside the chamber.
>
> Here is my recipe:
> -2000 rpm - 60 s
> -removing edge bead with Acetone, while spinning.
> -Soft bake at 110 C for 90 s
> -2000 rpm - 60 s
> -Soft bake at 110 C for 240 s.
>
> -Exposure, broadband source,950 mJ/cm2.
> -Developer, AZ400:DI 4:1, 3-4 mins.
> With this recipe, I am getting ~25 um. but when I put it inside DRIE,the
> resist is just peeling of and forming flakes.
>
> Can you please advise if there is something I am missing?
> Also, any recipe would be much appreciated.
>
> kind regards,
> Ajymurat
> _______________________________________________
> Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> provider of MEMS and Nanotechnology design and fabrication services.
> Visit us at http://www.mems-exchange.org
>
> Want to advertise to this community?  See http://www.memsnet.org
>
> To unsubscribe:
> http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>
_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation
Tanner EDA by Mentor Graphics